ZnO-Bi203-based varistor ceramics prepared by direct high-energy ball milling of the dopants Dong Xu1'2'*, Biao Wang lb , Mingshuang Li1'0, Xiao Ye l d 1.School of Material Science and Engineering, Jiangsu University, Zhenjiang 212013, P. R. China 2.Key Laboratory of Semiconductor Materials Science, Institute of Semiconductors, Chinese Academy of Sciences, Beijing 100083, P.R. China [email protected]; b. [email protected]; c. [email protected]; d. [email protected] electrical

addition of Sb 2 0 3 results in the formation of the

properties of ZnO-Bi203-based varistor ceramics

Zn7Sb20i2 spinel-type phase, to which the inhibition of

prepared by direct high-energy ball milling of the

the grain growth is generally assigned. Oxides of Co, Mn

dopants were studied. The varistor ceramics samples

and Ni incorporate into the grains of ZnO and increase

were characterized by XRD and SEM analysis, as

their conductivity. Hence, an optimum distribution of the

well as by dc electrical measurements, such as the

dopants has to be achieved in the ZnO matrix, both along

nonlinearity

the grain boundaries and in the grains in order to obtain

Abstract—The

microstructure

coefficients,

and

leakage

current

and

threshold voltage. The best electrical characteristics

the best functional

were found in sample P2, which exhibited the

ceramics. The homogeneity of the starting oxide mixture

threshold

voltage

was

347

V/mm,

is therefore of key importance for the preparation of

nonlinear

high-quality varistor ceramics[4_7].

coefficient was 39.2 and leakage current was 0.18 uA. Keywords-varistors; ZnO; high-energy ball milling;

Typically, the standard varistor ceramic procedure

microstructure; electrical properties I.

characteristics of the varistor

of mixing ZnO with varistor dopants is used for the processing of varistor ceramics. The high-energy ball

INTRODUCTION

milling of varistor powder can improve ZnO varistor

ZnO varistor ceramics show a highly nonlinear

characteristics,

providing

the

narrow

grain

size

current-voltage characteristic with a highly resistive

distribution, homogenous distribution of phases and high

state in the prebreakdown region and large non-linearity

sintering activity of the powders[ ' . It was also reported

2]

coefficient^' . The zinc oxide based varistors are widely

that mechanical activation reduces the weight loss due to

used in electronic appliances and especially in high

the volatilization of B12O3 and Sb203[ . In this work the

voltage lines as voltage surge protection devices.

dopants of varistor ceramics by high-energy ball milling

Commercial varistors are usually made by solid state of

firstly, then milled with ZnO powder, the influence of

ZnO particles with doping agent oxides such as Bi 2 0 3 ,

the different ball milling process on the microstructure

Sb203, C02O3, Mn02 and Cr203, the mixed powder then

development,

being pressed and sintered at higher temperatures^

current-voltage

.

the

phase

characteristics

composition of varistor

and

the

ceramics

Each of the dopants added to the ZnO powder play a

prepared by the high-energy ball milling method was

distinctive role in providing the varistor characteristics to

thoroughly analyzed.

the sintered ZnO-based ceramics. B12O3 is essential for II.

inducing the nonlinearity to the ZnO ceramics. Sb203 is a standard additive for controlling the grain growth. The

978-l-61284-088-8/ll/$26.00 ©2011 IEEE

EXPERIMENTAL PROCEDURE

The varistor dopant powder mixture, marked as DP,

713

12-14 August, 2011

which were used in reagent-grade raw materials in

III.

RESULTS AND DISCUSSION

proportions of 0.7 mol% Bi 2 0 3 , 1.0 mol% Sb 2 0 3 , 0.8

Fig. 1 shows the microstructures of the samples (PI, P2,

mol% Co 2 0 3 , 0.5 mol% Cr 2 0 3 and 0.5 mol% Mn0 2 , and

P3 and P4) sintered at 1100 °C for 2 h. A similar

the mixture were homogenized in absolute ethanol media

microstructure of the samples obtains in all cases with

in a polyethylene bowl with zirconia balls for 5 h at 500

the only appreciable difference coming from the average

rpm by planetary high-energy ball milling. Then the

size of ZnO grains, the microstructure of varistor

powder samples (3.5 mol% DP + 96.5 mol% ZnO) were

ceramics typically consists of three phases: ZnO grain,

ball milling with 0 h at 500 rpm (instead withl h at 100

spinel, and an intergranular Bi-rich phase as determined

rpm), 1 h at 500 rpm, 5 h at 500 rpm, 10 h at 500 rpm by

by X-ray diffraction (XRD) analysis. The 5h-milling

marked as PI, P2, P3 and P4, respectively.

sample has the smallest grains, and its grain interstice

The slurry was dried at 70 °C for 24h, it was then

phase (spinel phase) as well as grain boundary phase

pulverized by an agate mortar/pestle and after 2 wt.%

(Bi-rich phase) are more refined.

polyvinyl alcohol (PVA) binder had been added, it was

The influence of the high-energy ball milling on the

granulated by sieving through a 100-mesh screen to

characteristics, including the density D, the threshold

produce the starting power. The powders were then dried

voltage Vj, the nonlinear coefficient a, and the leakage

and pressed into discs with a diameter of 12 mm and a

current 7L of the ZnO-Bi203-based varistor ceramics

thickness of 2.0 mm. The pressed disks were sintered in

sintered at 1100 °C for 2 h are presented in Table 1.

air at 1100 °C (2h dwell time), using a heating rate of 5 °C/min and then cooled in the furnace. The sintered

Table 1 Density and electrical properties of

samples were lapped and polished to 1.0 mm thickness.

ZnO-Bi 2 0 3 -based varistor ceramics

The final samples were about 10 mm in diameter and 1.0 mm in thickness. The surface microstructure was examined by a scanning electron microscope (SEM, FEI QUANTA 400). The crystalline phases were identified by an X-ray diffractometry (XRD, Rigaku D/max 2200, Japan) using a Cu Ka radiation. The bulk density of the samples was measured in terms of their weight and

D (%)

IL (uA)

VT (V/mm)

q

PI

94.9

0.08

232

36.2

P2

97.4

0.18

347

39.2

P3

96.7

0.07

290

29.6

P4

96.6

0.05

279

36.6

Differential thermal and high temperature X-ray

volume. For the characterization of DC current-voltage,

analysis have recently suggested the following reactions

the silver paste was coated on both faces of samples and

for the microstructure development of ZnO varistor

the silver electrodes were formed by heating at 600 °C

during reactive liquid phase sintering in the temperature

for 10 min. The electrodes were 5 mm in diameter. The voltage-current (V-I)

Sample

range 500-1050°C[1415].

characteristics were measured

Sb 2 0 3 (s)+0 2 ^Sb 2 0 5 (l)

using a V-I source/measure unit (CJP CJ1001). The

Sb 2 0 5 (l)+ZnO(s)^ZnSb 2 0 6 (s)

nominal varistor voltages (KN) at 0.1 and 1.0 mA were

527 °C

700-800 °C

ZnSb 2 0 6 (s)+6ZnO(s)^Zn 7 Sb 2 Oi 2 (s)

measured and the threshold voltage Vj (V/mm) (Vj =

(1) (2)

6^800°C (3)

3ZnSb 2 0 6 (s)+3Bi 2 0 3 (s)+ZnO(s)^2Zn 2 Bi 3 Sb 3 Oi 4 (s)

V^(lmA)/d; d is the thickness of the sample in mm) and

700°C